GB713-2014 Q345R化學成分:
標準
年號 牌號 化學成分,(質(zhì)量分數(shù))% 其他
C Si Mn Cu Ni Cr Mo Nb V Ti Alt P S
GB713-2008 Q345R ≤
0.20 ≤
0.55 1.20
~
1.60 ≥
0.020 ≤
0.025 ≤
0.015 2008
GB713-2014 Q345R ≤
0.20 ≤
0.55 1.20
~
1.60 ≤
0.30 ≤
0.30 ≤
0.30 ≤
0.08 ≤
0.040 ≤
0.020 ≤
0.030 ≤
0.025 ≤
0.010 Cu+Ni+Cr+Mo≤
0.70
GB713-2014 Q345R力學性能:
鋼板厚度mm 抗拉強度Rm 屈服強度Re 伸長率A% 溫度 沖擊功KV2/J 彎曲試驗180°b=2a
>3-16 510-640Mpa ≥345Mpa 21 0°C,-20°C 41 KV2/J d=2a
>16-36 500-630Mpa ≥325Mpa 21 0°C,-20°C 41 KV2/J d=3a
>36-60 490-620Mpa ≥315Mpa 21 0°C,-20°C 41 KV2/J d=3a
>60-100 390-510Mpa ≥305Mpa 20 0°C,-20°C 41 KV2/J d=3a
>100-150 480-610Mpa ≥285Mpa 20 0°C,-20°C 41 KV2/J d=3a
>150-200 470~600Mpa ≥265Mpa 20 0°C,-20°C 41 KV2/J d=3a
GB713-2014 Q345R與歐標、美標相近材質(zhì)對照
標準 GB713-2014 EN10028-2:2009 ASME(2013) IS08328-2:2011附錄A(歐洲) IS08328-2:2011附錄B(美、日)
鋼號 Q345R P355GH SA516Gr.70 P355GH PT480GH
P % ≤0.025 ≤0.025 ≤0.035 ≤0.025 ≤0.025
S ≤0.010 ≤0.010 ≤0.035 ≤0.010 ≤0.025
KV2/J 0°C,≥41
-20°C,≥41 0°C,≥34
-20°C,≥27 系附加要求 0°C,≥34
-20°C,≥27 雙方協(xié)商
可協(xié)商40J 可協(xié)商40 |
 |
|